0.9620 Mould Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
Category | Type | Steel Grade | Standard | Country | Application |
---|---|---|---|---|---|
Steel Grades | Mould Steel | 0.9620 | |||
1.4569 |
|||||
GX3CrNiMoCuN24-6-5 |
|||||
1.4573 |
|||||
GX10CrNiCuNb18-12 |
|||||
1.4583 |
|||||
GX7CrNiMoCuNb18-8 |
|||||
1.4585 |
|||||
G-X300NiMo3Mg |
|||||
0.9610 |
|||||
G-X260NiCr4-2 |
C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
---|---|---|---|---|---|---|
2.6-2.9 | 0.2-0.8 | 0.3-0.7 | 1.4-2.4 | 3.3-5.0 | ||
Mo | Al | Cu | Nb | Ti | V | Ce |
≤0.5 | ||||||
N | Co | Pb | B | Other | ||
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
472 (≥) | 123 (≥) | 31 | 23 | 11 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 234 |
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
24 | - | - | 0.13 | - | |||
334 | 564 | - | 24.3 | 144 | - | ||
443 | - | 14 | 43.2 | 312 | 331 |
Heat treated : 1538°C - 1226°C