Germany DIN DIN EN 10088-1, DIN EN 10269, DIN EN 10302 (2002), 2.4669 Superalloys NiCrFeTi alloy; High-temperature resisting material and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.

Datasheet for: Steel Grades:Superalloys: 2.4669
Category Class Grade Standard Country Application
Steel GradesSuperalloys 2.4669 DIN Germany NiCrFeTi alloy; High-temperature resisting material

Chemical composition(mass fraction)(wt.%) of the 2.4669

C Mn Si S P Cu Fe Co Nb Cr Ni Al Ti
≤0.08 ≤1.0 ≤0.5 ≤0.01 ≤0.015 ≤0.5 5.0 -9.0 ≤1.0 0.70 -1.20 14.0 -17.0 70 - ≥ 0.40 -1.00 2.25 -2.75

Mechanical Properties of steel grade 2.4669

Yield
Rp0.2 (MPa)
Tensile
Rm (MPa)
Impact
KV/Ku (J)
Elongation
A (%)
Reduction in cross section on fracture
Z (%)
As-Heat-Treated Condition Brinell hardness (HBW)
696 (≥) 578 (≥) 34 12 13 Solution and Aging, Annealing, Ausaging, Q+T,etc 343

Physical Properties of steel grade 2.4669

Temperature
(°C)
Modulus of elasticity
(GPa)
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and Thermal conductivity
(W/m·°C)
Specific thermal capacity
(J/kg·°C)
Specific electrical resistivity
(Ω mm²/m)
Density
(kg/dm³)
Poisson’s coefficient, ν
22 - -     0.34 -  
582 423 - 21.3 233   -  
932 - 43 31.2   313 113

Heat Treatment of steel grade 2.4669

Heat treated : 1656°C - 1865°C

Technological Curves of steel grade 2.4669

Cross Reference Table (Equivalent Grade) of 2.4669

Relevant standard of 2.4669

DIN EN 10088-1 Stainless steels - Part 1: List of stainless steels DIN-EN-10088-1.pdf
DIN EN 10269 Steels and nickel alloys for fasteners with specified elevated and/or low temperature properties DIN-EN-10269.pdf
DIN EN 10302 (2002) Creep resisting steels, nickel and cobalt alloys DIN-EN-10302-(2002).pdf

Available Suppliers

Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...

Rfq.: sales@longhaisteel.com
  • Do you supply this 2.4669?
  • List your company on S&G now? Join
  • Non-paying users only
Top