France AFNOR NF A 35-595, Z100CD17CI Specialsteel Iron and steel. Cutlery stainless steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
Category | Class | Grade | Standard | Country | Application |
---|---|---|---|---|---|
Steel Grades | Specialsteel | Z100CD17CI | AFNOR | France | Iron and steel. Cutlery stainless steel |
C | Si | Mn | P | S | Cr | Mo | Ni |
---|---|---|---|---|---|---|---|
0.95 -1.20 | ≤1.00 | ≤1.00 | ≤0.040 | ≤0.015 | 16.00 -18.00 | 0.40 -0.80 | ≤ ≥ |
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
887 (≥) | 985 (≥) | 42 | 33 | 11 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 313 |
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
12 | - | - | 0.11 | - | |||
222 | 249 | - | 23.3 | 324 | - | ||
135 | - | 43 | 23.2 | 222 | 443 |
Heat treated : 1191°C - 1814°C
Grade | Standard | Country | Application |
---|---|---|---|
Z100CD17CI | |||
Z100CD17CI |
NF A 35-595 | Iron and steel. Cutlery stainless steel | NF-A-35-595.pdf |