USA AISI 17-4PH Stainless Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
Category | Type | Steel Grade | Standard | Country | Application |
---|---|---|---|---|---|
Steel Grades | Stainless Steel | 17-4PH | AISI | USA | |
ASTM 5140 |
|||||
AISI 201 |
|||||
AISI 202 |
|||||
00Cr12 |
|||||
0Cr13Al |
|||||
1Cr21Ni5Ti |
|||||
00Cr18Ni5Mo3Si2 |
|||||
1Cr18Ni11SiA1Ti |
|||||
0Cr26Ni5Mo2 |
|||||
410CB |
TYPICAL ANALYSIS |
|
|||||||
C. |
Mn. |
P. |
S. |
Si. |
Cr. |
Ni. |
Cu. |
Nb.+Ta.. |
0.07% |
1.00% |
0.04% |
0.03% |
1.00% |
15.00- |
3.00- |
3.00- |
0.15- |
Solution Treatments.
As supplied 17-4PH is usuall in the solution treated condition (Condition A). It can be heat treated at different temperatures to offer a wide range of properties. (We also hold stock in H1150+H1150, and annealed block).
Condition |
Hardening |
Hardening |
Type of Cooling |
Hardness |
|
|
Temperature |
Time |
|
Brinell |
Rockwell C |
A |
1038°C |
1/2 |
Oil/Air (to below 32°C) |
363 max. |
39 max. |
H900 |
480°C |
1 |
Air |
420 |
44 |
H925 |
495°C |
4 |
Air |
409 |
42 |
H1025 |
550°C |
4 |
Air |
352 |
38 |
H1075 |
580°C |
4 |
Air |
341 |
36 |
H1100 |
595°C |
4 |
Air |
332 |
35 |
H1150 |
621°C |
4 |
Air |
311 |
33 |
|
|
|
|
|
|
|
|
|
|
|
|
Typical Mechanical Properties (longitudinal)
|
A |
H900 |
H925 |
H1025 |
H1075 |
H1100 |
H1150 |
H1150+ |
H1150M |
Tensile Strength |
1034 |
1380 |
1310 |
1170 |
1140 |
1035 |
1000 |
965 |
860 |
0.2% YS |
760 |
1275 |
1200 |
1140 |
1035 |
930 |
860 |
760 |
585 |
Reduction of Area |
30-60 |
50 |
54 |
56 |
58 |
58 |
60 |
60 |
68 |
Elongation |
6-15 |
14 |
14 |
15 |
16 |
17 |
19 |
20 |
22 |
Charpy Impact |
- |
20 |
34 |
47 |
54 |
61 |
68 |
108 |
135 |
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
325 (≥) | 255 (≥) | 44 | 31 | 43 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 122 |
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
32 | - | - | 0.44 | - | |||
436 | 219 | - | 42.3 | 314 | - | ||
583 | - | 43 | 32.2 | 132 | 121 |
Heat treated : 1821°C - 1175°C
Grade | Standard | Country | Application |
---|---|---|---|
17-4PH | USA | Martensitic special steel | |
17-4PH | USA | Martensitic special steel |
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...