GX30CrSi7 Mould Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
Category | Type | Steel Grade | Standard | Country | Application |
---|---|---|---|---|---|
Steel Grades | Mould Steel | GX30CrSi7 | |||
G-X6CrNi18-9 |
|||||
1.4308 |
|||||
G-X5CrNiNb18-9 |
|||||
1.4552 |
|||||
G-X5CrNiMoNb18-10 |
|||||
1.4581 |
|||||
G-X6CrNiMo18-10 |
|||||
1.4408 |
|||||
G-X6CrNiMoN17-13-5 |
|||||
1.4439 |
C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
---|---|---|---|---|---|---|
0.20-0.35 | 1.00-2.50 | 0.50-1.50 | 0.035 | 0.030 | 6.00-8.00 | ≤ 0.50 |
Mo | Al | Cu | Nb | Ti | V | Ce |
≤ 0.15 | ||||||
N | Co | Pb | B | Other | ||
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
223 (≥) | 987 (≥) | 41 | 13 | 12 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 423 |
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
31 | - | - | 0.24 | - | |||
826 | 861 | - | 32.3 | 413 | - | ||
271 | - | 12 | 11.2 | 423 | 412 |
Heat treated : 1332°C - 1638°C
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...