C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
|---|---|---|---|---|---|---|
| 0.20-0.28 | 0.30-0.50 | 0.50-0.80 | 0.030 | 0.030 | ≤0.30 | |
| Mo | Al | Cu | Nb | Ti | V | Ce |
| N | Co | Pb | B | Other | ||
| ≤ 0.07 | ||||||
| Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
|---|---|---|---|---|---|---|
| 446 (≥) | 771 (≥) | 31 | 13 | 12 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 124 |
| Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
|---|---|---|---|---|---|---|---|
| 11 | - | - | 0.23 | - | |||
| 324 | 146 | - | 42.3 | 134 | - | ||
| 655 | - | 34 | 42.2 | 432 | 321 |
Heat treated : 1226°C - 1442°C