St37-3U Carbon Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
Category | Type | Steel Grade | Standard | Country | Application |
---|---|---|---|---|---|
Steel Grades | Carbon Steel | St37-3U | |||
S185 |
|||||
St33 |
|||||
1.0035 |
|||||
1.0038 |
|||||
RSt37-2 |
|||||
S235JR |
|||||
S235JR |
|||||
RSt37-2 |
|||||
1.0038 |
|||||
1.0114 |
C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
---|---|---|---|---|---|---|
0.17 | 1.40 | 0.030 | 0.030 | |||
Mo | Al | Cu | Nb | Ti | V | Ce |
≤ 0.55 | ||||||
N | Co | Pb | B | Other | ||
≤ 0.012 | tuoyang N | |||||
C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
---|---|---|---|---|---|---|
Mo | Al | Cu | Nb | Ti | V | Ce |
N | Co | Pb | B | Other | ||
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
448 (≥) | 194 (≥) | 14 | 13 | 22 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 244 |
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
41 | - | - | 0.23 | - | |||
244 | 959 | - | 24.3 | 431 | - | ||
881 | - | 41 | 42.2 | 242 | 231 |
Heat treated : 1731°C - 1787°C
Our main peoducts of steel are many kinds of special steel, like tool steel, mould steel, alloy steel, alloy constructural steel, heat-resistant steel, high speed tool steel,spring steel and bearing steel , stainless steel and so on, which have formed 12 series and more than 350 varieties with n...
Rfq.: sales@longhaisteel.com