FCDA-NiSiCr30-5-5 Carbon Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
Category | Type | Steel Grade | Standard | Country | Application |
---|---|---|---|---|---|
Steel Grades | Carbon Steel | FCDA-NiSiCr30-5-5 | |||
FCDA-NiMn13-7 |
|||||
FCDA-NiCr20-2 |
|||||
FCDA-NiCrNb20-2 |
|||||
FCDA-NiCr20-3 |
|||||
FCDA-NiSiCr20-5-2 |
|||||
FCDA-Ni22 |
|||||
FCDA-NiMn23-4 |
|||||
FCDA-NiCr30-1 |
|||||
FCDA-NiCr30-3 |
|||||
FCDA-NiSiCr30-5-2 |
C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
---|---|---|---|---|---|---|
2.6 | 5.0-6.0 | 0.5-1.5 | 4.5-5.5 | 28-32 | ||
Mo | Al | Cu | Nb | Ti | V | Ce |
≤0.5 | ||||||
N | Co | Pb | B | Other | ||
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
296 (≥) | 334 (≥) | 33 | 12 | 33 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 423 |
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
43 | - | - | 0.11 | - | |||
831 | 838 | - | 43.3 | 443 | - | ||
118 | - | 24 | 24.2 | 332 | 333 |
Heat treated : 1575°C - 1365°C