| Steel grade(ASTM) | HBS | Heat treatment | Quenching hardness ≥HRC | |||
| Annealing | Hard drawn | C % | Quenching temperature ℃ | Cooling medium | ||
| W1 | 202 | 241 | 0.70~0.85 | 802 | Brine | 64 | 
| W1 | 202 | 241 | 0.85~0.95 | 802 | Brine | 65 | 
| W1 | 202 | 241 | 0.95~1.50 | 788 | Brine | 65 | 
| W2 | 202 | 241 | 0.85~0.95 | 802 | Brine | 65 | 
| W2 | 202 | 241 | 0.95~1.50 | 788 | Brine | 65 | 
| W5 | 202 | 241 | 1.05~1.15 | 802 | Brine | 65 |