1.6740 Mould Steel and Mechanical Properties, Chemical Element, Cross Reference, Datasheet.
Category | Type | Steel Grade | Standard | Country | Application |
---|---|---|---|---|---|
Steel Grades | Mould Steel | 1.6740 | |||
1.6552 |
|||||
GS-24CrNiMo3-2-5 |
|||||
1.6552 |
|||||
G34CrNiMo6 |
|||||
1.6582 |
|||||
GS-34CrNiMo6 |
|||||
1.6582 |
|||||
G33CrNiMo7-4-4 |
|||||
1.6740 |
|||||
GS-33CrNiMo7-4-4 |
C ≤ |
Si ≤ |
Mn ≤ |
P ≤ |
S ≤ |
Cr | Ni |
---|---|---|---|---|---|---|
0.30-0.36 | 0.60 | 0.50-0.80 | 0.015 | 0.007 | 0.90-1.20 | 1.50-1.80 |
Mo | Al | Cu | Nb | Ti | V | Ce |
0.35-0.50 | ||||||
N | Co | Pb | B | Other | ||
Yield Rp0.2 (MPa) |
Tensile Rm (MPa) |
Impact KV/Ku (J) |
Elongation A (%) |
Reduction in cross section on fracture Z (%) |
As-Heat-Treated Condition | Brinell hardness (HBW) |
---|---|---|---|---|---|---|
631 (≥) | 241 (≥) | 44 | 11 | 24 | Solution and Aging, Annealing, Ausaging, Q+T,etc | 432 |
Temperature (°C) |
Modulus of elasticity (GPa) |
Mean coefficient of thermal expansion 10-6/(°C) between 20(°C) and | Thermal conductivity (W/m·°C) |
Specific thermal capacity (J/kg·°C) |
Specific electrical resistivity (Ω mm²/m) |
Density (kg/dm³) |
Poisson’s coefficient, ν |
---|---|---|---|---|---|---|---|
12 | - | - | 0.14 | - | |||
352 | 933 | - | 22.3 | 423 | - | ||
348 | - | 22 | 32.2 | 444 | 423 |
Heat treated : 1486°C - 1144°C